Test report of vulcanized fiber sheet and vulcanized fiber roll test report

test report of vulcanized fiber sheet and vulcanized fiber roll test report :

VULCANIZED FIBRE INDEX DATA

The information below is believed to be accurate and reliable. Youngman co.assumes no responsibility for end-use applications and no performance warranty is expressed or implied. Values shown are typical, are not guaranteed, nor to be used for specifications without approval.

Properties  Thickness (inches) Units Commercial Bone Electrical
Density .062″ grams/cm3 1.20 1.30 1.20
Specific Volume .062″ in3/lb 23.0 21.0 23.0


Mechanical

Tensile Strength MD .062″ psi 16,000 19,000 18,000
CD .062″ psi 9,000 9,500 10,000
Modulus of Elasticity in Tension MD .062″ psi x 105 12.0 12.0 12.0
CD .062″ psi x 105 8.0 8.0 8.0
Flexural Strength MD .062″ psi 15,000 15,000 15,000
CD .062″ psi 13,000 13,000 13,000
Compressive Strength .062″ psi 35,000 35,000 35,000
Impact Strength, Izod Edgewise MD .062″ ft-lbs/in. notch 2.0 1.4 2.5
CD .062″ ft-lbs/in. notch 1.8 1.0 2.0
Hardness, Rockwell R Scale .062″ Divisions 80 100 70
Bond Strength, .062″ psi 900 1,500 900
Bursting Strength, Mullen .016″ psi 325
Tear Strength, Elmendorf MD .016″ grams 550
CD .016″ grams 700


Electrical

Dielectric Strength, Short Time .016″ volts/mil 230 300
.062″ volts/mil 200 200 215
.125″ volts/mil 195 200 200
Arc Resistance .062″ seconds 80 100 125


Physical

Thermal Conductivity, 149° F Btu/hr/ft2//ft. .168 .168 .168
Specific Heat Btu/lb/ .403 .403 .403
Heat Resistance, Continuous 230 – 240 230 – 240 230 – 240
Thermal Expansion x 10-5 MD   in/in/ 1.1 1.1 1.1
CD   in/in/ 1.7 1.7 1.7
Dimensional Change per % change in Moisture Content Thick.   % 1.00 1.00 1.00
MD   % 0.10 0.10 0.10
CD   % 0.25 0.25 0.25
Water Absorption, 24 hours .062″ % 66.0 55.0 63.0
Coefficient of Friction, Fibre
on Fibre
0.16 0.16 0.16
Coefficient of Friction, Fibre on Smooth Cast Iron 0.21 0.21 0.21
Flammability, .062″ in/mm 0.5 0.5 0.5